Case Study|Metal Contamination Removal

Customer test data

Wafer Metal Contamination Removal Test at a Power Device Maker: Ozone Microbubbles Plus Dilute HF Cut Cu, Fe, Ni and Al by 2–3 Orders of Magnitude

Metal contamination on wafers is conventionally removed with 80℃ hydrochloric acid–hydrogen peroxide (SC-2), followed by hot-water and ultrapure-water rinses. After switching to 60℃ ozone microbubbles, residual copper, iron, nickel and aluminum were measured before and after cleaning. The data comes from a trial evaluation a power device maker carried out on the premise of adoption.

SitePower device maker, wafer evaluation (anonymized)
ComparisonBefore cleaning vs. ozone microbubbles vs. ozone microbubbles + dilute HF
StatusTrial evaluation on the premise of adoption (2019)
Inside a cleaning chamber, a nozzle sprays a fine stream of water onto a spinning wafer
A single-wafer cleaner spraying cleaning liquid onto the wafer surface (AI illustration)
Ozone microbubbles only1/50Cu, Fe, Ni, Al cut to approx. 1/10–1/50 of initial
Ozone microbubbles + dilute HF1/3,700Below 1/100; nickel approx. 1/3,700
Cleaning process3→2Process steps, no hydrochloric acid or hydrogen peroxide

Key takeaways: how low can ozone microbubbles bring metal contamination?

In a power device maker's wafer evaluation, cleaning with ozone microbubbles alone brought copper, iron, nickel and aluminum down to approx. 1/10–1/50 of their initial levels (about one order of magnitude or more); adding a dilute hydrofluoric acid (DHF) step after the ozone microbubbles brought all four metals below 1/100 of initial — nickel approx. 1/3,700 and iron approx. 1/540 — a reduction of 2–3 orders of magnitude or more. The process we propose replaces 80℃ hydrochloric acid–hydrogen peroxide (SC-2) with 60℃ ozone microbubbles, cutting the steps from 3 to 2. These are test data from our customer; actual results must be confirmed with a controlled trial on your own wafers.

Why look for a new way to remove metal contamination?

Power devices must withstand high voltages and large currents; metal left on the wafer surface can form leakage paths and affect gate oxide reliability, so post-clean metal residue must be kept very low. The conventional method is SC-2 in RCA cleaning (hydrochloric acid + hydrogen peroxide + water, 80℃); for a full explanation of RCA cleaning, see “Dry cleaning vs wet cleaning”.

Metal contamination removal process: conventional vs. ozone microbubbles
ItemConventionalOzone microbubbles
ProcessSC-2 80℃ → hot-water rinse 80℃ → ultrapure-water rinseOzone microbubbles 60℃ → ultrapure-water rinse
Process steps32
ChemicalHydrochloric acid, hydrogen peroxideNo hydrochloric acid or hydrogen peroxide
Process temperature80℃60℃

The process comparison is our proposed alternative. The lowest metal residue in the evaluation came from adding a dilute HF step after the ozone microbubbles.

Results: all four metals decreased

The original chart uses a logarithmic scale (each gridline is a factor of 10). The table below converts it to values relative to the initial level — the smaller the number, the cleaner the wafer:

Metal residue relative to before cleaning (before cleaning = 1)
MetalBefore cleaningOzone microbubblesOzone microbubbles + dilute HF
Copper Cu1approx. 1/11approx. 1/95 or lower
Iron Fe1approx. 1/22approx. 1/540
Nickel Ni1approx. 1/50 or lowerapprox. 1/3,700 or lower
Aluminum Al1approx. 1/45 or lowerapprox. 1/400 or lower

Values were read from the original log-scale chart and are approximate; the pre-cleaning values for nickel and aluminum hit the top of the chart, so the actual reduction may be larger (hence “or lower”). Copper fell below the bottom of the chart after the dilute HF step. The original chart does not state units or measurement method.

Why does one dilute HF step make such a big difference?

Ozone is a strong oxidizer: it oxidizes the wafer surface together with the metals, forming a very thin oxide film in which some of the metal becomes trapped. Dilute hydrofluoric acid dissolves this thin oxide film, carrying the trapped metal away with it. So ozone microbubbles alone already achieve about one order of magnitude, and adding dilute HF takes it down a further 1–2 orders.

The oxidizing power of ozone microbubbles comes from hydroxyl radicals generated when the bubbles collapse; for a plain-language explanation, see “What is the hydroxyl radical”.

3 lessons from this data

  • First decide how low you need to go: ozone microbubbles alone cut about one order of magnitude; to go lower, the approach in the evaluation was to add dilute HF.
  • Each metal differs in difficulty: under the same conditions, iron and aluminum residues stayed higher than nickel and copper, so a trial should include the metals you care about most in its measurements.
  • Agree on the measurement method first: metal residue is commonly measured by total reflection X-ray fluorescence (TXRF) or vapor phase decomposition with inductively coupled plasma mass spectrometry (VPD-ICP-MS); agree on the method and pass criteria before the trial.

Data sources and limitations

The data on this page is test data from our customers' evaluation period (c. 2019), when the evaluations were still in progress; customer names are withheld under confidentiality.

Figures were read from the original charts and are approximate. DEYly has not independently retested them, and actual results will vary with contaminants, materials, equipment and process conditions; before adopting, please confirm with a controlled trial on your own samples.

FAQ

Can ozone microbubbles remove metal contamination from wafers?

Yes. In a power device maker's evaluation, cleaning with ozone microbubbles alone brought copper, iron, nickel and aluminum down to approx. 1/10–1/50 of initial levels; adding dilute hydrofluoric acid (DHF) brought all four metals below 1/100, with nickel at approx. 1/3,700.

Why add a dilute HF step?

Ozone oxidizes the wafer surface and the metals into a thin oxide film, trapping some metal inside it. Dilute hydrofluoric acid dissolves the film and carries the metal away with it, so residue drops a further 1–2 orders of magnitude.

Can ozone microbubbles replace SC-2 (hydrochloric acid–hydrogen peroxide)?

The process we propose uses 60℃ ozone microbubbles plus an ultrapure-water rinse to replace 80℃ SC-2 and the hot-water rinse, cutting the steps from 3 to 2 with no hydrochloric acid or hydrogen peroxide. Whether it fits depends on your device's metal residue requirements; we recommend a controlled trial first.

Which power device maker's data is this?

Customer names are withheld under confidentiality. This is our customer's evaluation data from c. 2019, when the maker was running a trial evaluation on the premise of adoption.

Your turn